A half-wave plate is an exact half-wave plate at only one wavelength. Waveplate Principles: How Half-Wave and Quarter-Wave Plates Convert Polarization worked through an example: a zero-order half-wave plate designed for 550 nm, when used at 450 nm, retains a polarization conversion efficiency of only about 88% even if material dispersion is ignored. White-light imaging, multispectral measurement, full-color displays and broadband laser systems all need the same polarization conversion over a range of wavelengths. A single plate cannot provide this, and that is exactly the problem achromatic waveplates solve.

An achromatic waveplate is a compound retarder whose phase retardation stays approximately constant over a range of wavelengths. There are three main approaches to making one: letting two materials with different dispersions compensate each other; stacking several plates of the same material at specific angles so that the errors of the individual plates cancel geometrically, with multilayer twisted liquid crystal polymer structures being a continuous version of this idea; and directly using a material whose birefringence varies anomalously with wavelength. This article first analyzes why retardation varies with wavelength and explains why a single plate cannot be made achromatic, then discusses each of these methods in turn, the specifications used to evaluate them, and their relation to broadening the bandwidth of geometric phase devices.

This article follows the notation of that article. The time factor is e−iωte^{-i\omega t}; the Jones matrix of a waveplate with its fast axis along xx is W(Γ)=diag(1,eiΓ)W(\Gamma)=\mathrm{diag}(1,e^{i\Gamma}). Circular handedness follows the convention of Hecht's Optics: looking toward the oncoming light, a clockwise-rotating field is right-handed and a counterclockwise one is left-handed [1], and the Jones vector of left-handed light is 12(1, i)T\tfrac{1}{\sqrt2}(1,\ i)^{\mathsf T}. On the Poincaré sphere, the north pole L represents left-handed polarization, the south pole R represents right-handed polarization, and the equator holds linear polarizations of all orientations.

To judge a half-wave plate, this article mainly uses one quantity: for circularly polarized input, the fraction η\eta of the intensity converted to the opposite handedness. For a single plate with retardation Γ\Gamma, η=sin⁡2(Γ/2)\eta=\sin^2(\Gamma/2), and the "leakage" that is not converted and keeps its original handedness is 1−η=cos⁡2(Γ/2)1-\eta=\cos^2(\Gamma/2). Writing the retardation error as ε=Γ−π\varepsilon=\Gamma-\pi, for small errors 1−η≈ε2/41-\eta\approx\varepsilon^2/4: the leakage grows with the square of the error.

Why retardation varies with wavelength

A waveplate of thickness dd and birefringence Δn\Delta n has a phase retardation of

Γ(λ)=2π Δn(λ) dλ\Gamma(\lambda)=\frac{2\pi\,\Delta n(\lambda)\,d}{\lambda}

where λ\lambda is the vacuum wavelength. Two factors in this expression vary with wavelength. The first is λ\lambda in the denominator: the same optical path difference Δn d\Delta n\,d is a larger fraction of a short wavelength and therefore corresponds to more phase. This term is independent of the material and is present in every waveplate. The second is the dispersion of the birefringence itself, Δn(λ)\Delta n(\lambda), which depends on the material.

The relative contributions of the two factors can be seen by differentiating ln⁡Γ\ln\Gamma. With ln⁡Γ=ln⁡(2πd)+ln⁡Δn−ln⁡λ\ln\Gamma=\ln(2\pi d)+\ln\Delta n-\ln\lambda, differentiating with respect to ln⁡λ\ln\lambda gives

λΓdΓdλ=−1+λΔndΔndλ=−ΔngΔn,Δng=Δn−λdΔndλ\frac{\lambda}{\Gamma}\frac{\mathrm{d}\Gamma}{\mathrm{d}\lambda}=-1+\frac{\lambda}{\Delta n}\frac{\mathrm{d}\Delta n}{\mathrm{d}\lambda}=-\frac{\Delta n_g}{\Delta n},\qquad \Delta n_g=\Delta n-\lambda\frac{\mathrm{d}\Delta n}{\mathrm{d}\lambda}

Δng\Delta n_g is called the group birefringence; it has the same form as the group index ng=n−λ dn/dλn_g=n-\lambda\,\mathrm{d}n/\mathrm{d}\lambda. The left-hand side is "the percentage change in retardation for a 1% change in wavelength". The −1-1 comes from the 1/λ1/\lambda factor; the second term comes from material dispersion. In the transparent region, the birefringence of common materials decreases as the wavelength increases, dΔn/dλ<0\mathrm{d}\Delta n/\mathrm{d}\lambda<0, so the second term is also negative and adds to the first with the same sign, making Δng\Delta n_g larger than Δn\Delta n.

Calculated from dispersion equations in the literature, at 550 nm Δng/Δn≈1.10\Delta n_g/\Delta n\approx1.10 for quartz [2] and about 1.046 for magnesium fluoride (MgF₂) [3]. The dispersion of liquid crystal materials is usually much stronger: the polymerizable liquid crystal RMS10-025 used by Komanduri et al. has a birefringence of Δn(λ)=0.128+8390/λ2\Delta n(\lambda)=0.128+8390/\lambda^2 (λ\lambda in nm) [4], from which Δn=0.156\Delta n=0.156 and Δng/Δn≈1.36\Delta n_g/\Delta n\approx1.36 at 550 nm. In other words, for every 1% change in wavelength, the retardation of a quartz waveplate changes by about 1.1%, while that of this liquid crystal layer changes by about 1.36%.

Δng\Delta n_g also has a more direct physical meaning. Writing the retardation as a function of angular frequency ω\omega, Γ=ω Δn d/c\Gamma=\omega\,\Delta n\,d/c, where cc is the speed of light in vacuum, and differentiating with respect to ω\omega gives dΓ/dω=Δngd/c\mathrm{d}\Gamma/\mathrm{d}\omega=\Delta n_g d/c. The right-hand side is exactly the difference Δτ\Delta\tau between the group delays of the slow-axis and fast-axis components through the plate. Near the center frequency ω0\omega_0, therefore,

Γ(ω)≈Γ(ω0)+Δτ (ω−ω0)\Gamma(\omega)\approx\Gamma(\omega_0)+\Delta\tau\,(\omega-\omega_0)

The slope of retardation versus frequency is the group delay difference between the two polarization components. If the two components reach the exit face at different times, their phase difference cannot be the same for all frequencies. This gives achromatic design a clear goal: at the design frequency, the phase difference between the two components equals π\pi (or π/2\pi/2), and the group delay difference equals zero.

Example. Using Ghosh's dispersion equation for quartz [2], Δn=0.00916\Delta n=0.00916 at 550 nm, and a zero-order half-wave plate has thickness d=λ/(2Δn)≈30.0 μmd=\lambda/(2\Delta n)\approx30.0\ \mu\mathrm{m}. At 450 nm its retardation is 1.252π1.252\pi, or 1.222π1.222\pi if dispersion is ignored and only the 1/λ1/\lambda factor is counted; at 700 nm the two values are 0.770π0.770\pi and 0.786π0.786\pi. Taking η≥0.99\eta\ge0.99 as the criterion, the usable range of this quartz half-wave plate is 520.5–584 nm, or 517.5–587 nm if dispersion is ignored. For quartz, the wavelength dependence comes mainly from the 1/λ1/\lambda factor, and material dispersion only makes things slightly worse.

Retardation versus wavelength for single and two-material half-wave plates
Figure 1. Phase retardation Γ/π\Gamma/\pi versus wavelength for half-wave plates designed for 550 nm (example calculation). The black line is a single zero-order quartz half-wave plate, the grey dashed line is the case with only the 1/λ1/\lambda factor and dispersion ignored, and the red line is the quartz and MgF₂ two-material achromatic combination discussed below. The light red band is the retardation range ∣Γ−π∣≤0.2 rad|\Gamma-\pi|\le0.2\ \mathrm{rad} corresponding to η≥0.99\eta\ge0.99. The birefringence of quartz and MgF₂ is calculated from dispersion equations in the literature [2][3].

Why a single plate cannot be achromatic

For the retardation to be independent of wavelength near λ0\lambda_0, we need dΓ/dλ=0\mathrm{d}\Gamma/\mathrm{d}\lambda=0. From the expression in the previous section, this is equivalent to Δng(λ0)=0\Delta n_g(\lambda_0)=0, that is,

dΔndλ=Δnλ\frac{\mathrm{d}\Delta n}{\mathrm{d}\lambda}=\frac{\Delta n}{\lambda}

The thickness dd has dropped out of the condition. Thickness determines only the magnitude of the retardation, not the relative slope of its variation with wavelength, so the condition cannot be met whether the single plate is made zero-order or multi-order; a multi-order plate has the same relative slope as a zero-order plate, while its absolute error is magnified by a factor of 2m+12m+1.

A material satisfying the condition must have a birefringence that increases in proportion to wavelength, Δn∝λ\Delta n\propto\lambda. This is the opposite of how most transparent materials behave: their operating band lies on the long-wavelength side of the ultraviolet electronic absorption bands, and the closer to an absorption band, the faster the refractive index rises; the rise also differs along and perpendicular to the optic axis, and the birefringence usually increases along with it, so Δn\Delta n increases as the wavelength decreases. Komanduri et al. also pointed out that the birefringence dispersion of almost all optical materials prevents a single plate from achieving broadband polarization transformation [4].

This points to three routes for achromatic design. The first is to divide the task between materials with different dispersions so that the total group delay difference is zero. The second keeps the material unchanged and instead combines several plates of the same material at specific angles, so that the errors of the plates cancel each other in polarization-state space. The third is to create an anomalously dispersive material whose Δn\Delta n increases approximately in proportion to wavelength, so that a single layer satisfies the condition by itself.

Two-material combinations: zeroing the group delay difference

Two waveplates of different materials are stacked with their optic axes perpendicular, so that their retardations subtract. The net optical path difference is R(λ)=d1Δn1(λ)−d2Δn2(λ)R(\lambda)=d_1\Delta n_1(\lambda)-d_2\Delta n_2(\lambda) and the net retardation is Γ=2πR/λ\Gamma=2\pi R/\lambda. At the design wavelength λ0\lambda_0, the combination must be a half-wave plate and dΓ/dλ=0\mathrm{d}\Gamma/\mathrm{d}\lambda=0. By the same derivation as for a single plate, the second condition is equivalent to a zero net group path difference:

d1Δn1−d2Δn2=λ02,d1Δng1−d2Δng2=0d_1\Delta n_1-d_2\Delta n_2=\frac{\lambda_0}{2},\qquad d_1\Delta n_{g1}-d_2\Delta n_{g2}=0

This is a system of linear equations in d1d_1 and d2d_2. From the second equation, d2=d1Δng1/Δng2d_2=d_1\Delta n_{g1}/\Delta n_{g2}; substituting into the first and introducing for each material the ratio ρi=Δni/Δngi\rho_i=\Delta n_i/\Delta n_{gi} gives

d1=λ0/2Δng1 (ρ1−ρ2),d2=d1 Δng1Δng2d_1=\frac{\lambda_0/2}{\Delta n_{g1}\,(\rho_1-\rho_2)},\qquad d_2=d_1\,\frac{\Delta n_{g1}}{\Delta n_{g2}}

The closer ρ\rho is to 1, the weaker the birefringence dispersion of the material. To obtain positive thicknesses, material 1 should be the one with the larger ρ\rho and weaker dispersion. The reasoning is similar to that of an achromatic doublet lens: the two materials have different dispersions, one provides the required "retardation" and the other cancels its dispersion. The closer the values of ρ\rho for the two materials, the smaller the denominator and the larger the required thicknesses.

Example. From the dispersion equations in the literature [2][3], at 550 nm ρ=0.909\rho=0.909 for quartz and ρ=0.956\rho=0.956 for MgF₂; MgF₂ has the weaker dispersion and is taken as material 1. Substituting into the expressions above gives an MgF₂ thickness of about 470 µm and a quartz thickness of about 578 µm, with the two optic axes orthogonal. Taken individually, the MgF₂ plate has a retardation of about 10.1 waves and the quartz plate about 9.6 waves; only their difference is half a wave. The red line in Figure 1 is the retardation curve of this combination: the curve flattens near 550 nm, and the range with η≥0.99\eta\ge0.99 widens from 520.5–584 nm for single quartz to 459–708 nm.

This design only sets the first derivative to zero, so the residual error grows parabolically as the wavelength departs from the design value; at 400 nm and 800 nm the retardation drops to 0.75π0.75\pi and 0.88π0.88\pi. Hariharan gave a systematic method for choosing material combinations that minimize the residual error, and pointed out that using three birefringent materials can almost completely eliminate the residual wavelength dependence; such combinations are called apochromatic retarders [5].

The cost of two-material combinations comes from their thickness. Each plate has a retardation of about 10 waves, so any change that does not cancel between them acts on the scale of 10 waves. At oblique incidence, the optical path and effective birefringence in each plate change by amounts proportional to thickness, and the changes in the two materials generally do not cancel exactly. Hale and Day analyzed compound zero-order waveplates made of a single material: their response to temperature and wavelength is the same as that of a true zero-order waveplate, but their response to the angle of incidence is the same as that of a multi-order waveplate of the same thickness; they also proposed combining a positive uniaxial crystal with a negative uniaxial crystal, which significantly reduces the sensitivity to the angle of incidence at the cost of slightly higher temperature sensitivity [6]. Komanduri et al. also noted that two-material combinations such as quartz and MgF₂ have a limited achromatic bandwidth and are sensitive to misalignment between the two plates, to temperature changes and to the angle of incidence [4].

Pancharatnam three-plate design: canceling errors with angles

In 1955, Pancharatnam published two papers on achromatic combinations of birefringent plates: the first used two half-wave plates and one quarter-wave plate to form an achromatic circular polarizer [7], and the second used three plates to form an achromatic quarter-wave plate [8]. All three plates are made of the same material, and he specifically pointed out that the birefringence dispersion of the material need not be small [8]. The compensation relies not on differences between materials but on the angles between the optic axes of the plates.

The principle is explained below using an achromatic half-wave plate as the example. Three identical half-wave plates are stacked in sequence, with the optic axes of the first and third plates parallel, taken as 0∘0^\circ, and the middle plate rotated by θ\theta (Figure 2a). The three plates are made of the same material with the same thickness, so at any wavelength they have the same retardation error ε(λ)\varepsilon(\lambda), regardless of whether the error comes from the 1/λ1/\lambda factor or from material dispersion.

Pancharatnam three-plate half-wave plate and error axes
Figure 2. Pancharatnam three-plate achromatic half-wave plate. (a) Three identical half-wave plates arranged in the order the light passes through them (viewed facing the light); thick lines show the optic axis of each plate: plates 1 and 3 at 0∘0^\circ, plate 2 rotated by θ\theta. Each plate has a retardation of π+ε(λ)\pi+\varepsilon(\lambda). (b) Equatorial plane of the Poincaré sphere (viewed from above the S3S_3 axis). The three arrows are the directions of the error rotation axes of the three plates after being transferred to the exit side; the numbers are plate numbers, and adjacent arrows are 2θ2\theta apart. At θ=60∘\theta=60^\circ the three are 120∘120^\circ apart and, placed head to tail, form a closed triangle with zero vector sum.

Error cancellation on the Poincaré sphere

As described in Waveplate Principles: How Half-Wave and Quarter-Wave Plates Convert Polarization, on the Poincaré sphere a waveplate with optic axis at φ\varphi and retardation Γ\Gamma rotates the polarization state by an angle Γ\Gamma about the equatorial axis at longitude 2φ2\varphi. A half-wave plate with retardation π+ε\pi+\varepsilon can be regarded as first rotating by π\pi about this axis and then rotating by an additional small angle ε\varepsilon about the same axis; two rotations about the same axis can be performed in either order.

When the three plates act in sequence, the small error rotation of each plate is sandwiched between ideal π\pi rotations. To see their total effect, all three small rotations are moved to the exit side. The move uses a geometric relation: let AA be any rotation; "first rotating by a small angle ε\varepsilon about the axis u\mathbf u, then applying AA" is equivalent to "first applying AA, then rotating by the same ε\varepsilon about the axis AuA\mathbf u carried along by AA". In other words, when an error rotation is moved past a later element, its rotation axis is carried to a new position by that element.

Apply this relation plate by plate. The error of plate 3 is already on the exit side, with its rotation axis at longitude 0∘0^\circ. The error rotation axis of plate 2 is originally at longitude 2θ2\theta and must be moved past the π\pi rotation of plate 3; a π\pi rotation about the equatorial axis at longitude 0∘0^\circ turns longitude LL on the equator into −L-L, so it arrives at the exit side at longitude −2θ-2\theta. The error rotation axis of plate 1 is originally at longitude 0∘0^\circ; it is first moved past plate 2, where the π\pi rotation about the axis at longitude 2θ2\theta carries it to longitude 4θ4\theta, and then past plate 3, which carries it to −4θ-4\theta. All three rotation axes remain on the equator.

To first order, the composition of small rotations is the sum of the rotation vectors. Each of the three error rotations has magnitude ε\varepsilon, so the total error is approximately ε\varepsilon times the sum of three unit vectors at longitudes 00, −2θ-2\theta and −4θ-4\theta. The sum of three vectors of equal length is zero only if they are 120∘120^\circ apart, that is, 2θ=120∘2\theta=120^\circ and θ=60∘\theta=60^\circ (Figure 2b). The first-order error then cancels completely, and only higher-order terms in ε\varepsilon remain. This derivation did not use the input polarization state, so the cancellation holds for any input polarization.

Figure 3 shows this with trajectories on the Poincaré sphere. Left-handed light starts at the north pole L, and the retardation of each plate is taken as 0.7π0.7\pi, a considerable error. With a single plate, the polarization state moves 126∘126^\circ along a meridian and stops, still 54∘54^\circ from the target, the south pole R. With three plates, plate 1 likewise goes halfway; plate 2 brings the polarization state back near the north pole, but the landing point is offset from the pole; plate 3 starts from this offset position and ends only 10.7∘10.7^\circ from the south pole. The role of the middle plate is to place the polarization state in the right position so that the error of plate 3 exactly makes up the shortfall of plate 1.

Poincare sphere trajectories for single and three-plate half-wave plates
Figure 3. Polarization-state trajectories on the Poincaré sphere for left-handed circularly polarized light passing through half-wave plates (example calculation, retardation per plate Γ=0.7π\Gamma=0.7\pi). L and R are the north pole (left-handed) and south pole (right-handed), and H is horizontal linear polarization; solid lines are on the front of the sphere and dashed lines on the back. (a) Single plate; the end point is about 54∘54^\circ from R. (b) Three plates arranged at 0∘/60∘/0∘0^\circ/60^\circ/0^\circ; 1, 2 and 3 are the trajectory segments of the respective plates, u2u_2 is the rotation axis of plate 2, and plates 1 and 3 rotate about the axis through point H; the end point is about 10.7∘10.7^\circ from R.

A quantitative treatment with Jones matrices

In his second paper, Pancharatnam proved that a three-plate combination in which the first and third plates have parallel optic axes and equal retardations is equivalent to a pure linear retarder, with an equivalent retardation Γeff\Gamma_{\mathrm{eff}} satisfying [8]

cos⁡Γeff2=cos⁡Γ1cos⁡Γ22−sin⁡Γ1sin⁡Γ22cos⁡2θ\cos\frac{\Gamma_{\mathrm{eff}}}{2}=\cos\Gamma_1\cos\frac{\Gamma_2}{2}-\sin\Gamma_1\sin\frac{\Gamma_2}{2}\cos2\theta

where Γ1\Gamma_1 is the retardation of each of the two outer plates, Γ2\Gamma_2 is the retardation of the middle plate, and θ\theta is the angle between the optic axes of the middle and outer plates. This result can be verified directly by multiplying the Jones matrices of the three plates in the order the light passes through them [9].

When all three plates are half-wave plates with retardation Γ\Gamma, Γ1=Γ2=Γ\Gamma_1=\Gamma_2=\Gamma. Substituting cos⁡Γ=cos⁡2(Γ/2)−sin⁡2(Γ/2)\cos\Gamma=\cos^2(\Gamma/2)-\sin^2(\Gamma/2) and sin⁡Γ=2sin⁡(Γ/2)cos⁡(Γ/2)\sin\Gamma=2\sin(\Gamma/2)\cos(\Gamma/2) and factoring out cos⁡(Γ/2)\cos(\Gamma/2) gives

cos⁡Γeff2=cos⁡Γ2[cos⁡2Γ2−(1+2cos⁡2θ)sin⁡2Γ2]\cos\frac{\Gamma_{\mathrm{eff}}}{2}=\cos\frac{\Gamma}{2}\left[\cos^2\frac{\Gamma}{2}-\left(1+2\cos2\theta\right)\sin^2\frac{\Gamma}{2}\right]

For a pure linear retarder, the leakage of circularly polarized light depends only on the equivalent retardation, 1−η=cos⁡2(Γeff/2)1-\eta=\cos^2(\Gamma_{\mathrm{eff}}/2), and not on the direction of the equivalent optic axis. Let Γ=π+ε\Gamma=\pi+\varepsilon; then cos⁡(Γ/2)=−sin⁡(ε/2)≈−ε/2\cos(\Gamma/2)=-\sin(\varepsilon/2)\approx-\varepsilon/2 and sin⁡(Γ/2)≈1\sin(\Gamma/2)\approx1. The leakage of a single plate is about (ε/2)2(\varepsilon/2)^2; for the three-plate combination the dominant term in the brackets is −(1+2cos⁡2θ)-(1+2\cos2\theta), and the leakage is about (ε/2)2(1+2cos⁡2θ)2(\varepsilon/2)^2(1+2\cos2\theta)^2. At θ=60∘\theta=60^\circ, 1+2cos⁡2θ=01+2\cos2\theta=0, only cos⁡2(Γ/2)\cos^2(\Gamma/2) remains in the brackets, and the leakage becomes

1−η=cos⁡6Γ2≈(ε2)61-\eta=\cos^6\frac{\Gamma}{2}\approx\left(\frac{\varepsilon}{2}\right)^6

This agrees with the conclusion on the Poincaré sphere: once the first-order error cancels, the leakage drops from the second power of the error to the sixth power.

Example. With a retardation of Γ=0.7π\Gamma=0.7\pi per plate, cos⁡(0.35π)=0.454\cos(0.35\pi)=0.454. The leakage of a single plate is 0.4542≈20.6%0.454^2\approx20.6\% and that of the three-plate combination is 0.4546≈0.88%0.454^6\approx0.88\%, corresponding to the end points 54∘54^\circ and 10.7∘10.7^\circ from the south pole in Figure 3.

Why 58° is often used instead of 60°

θ=60∘\theta=60^\circ makes the error curve flattest near the design wavelength, but it does not give the widest usable band. If θ\theta is slightly less than 60∘60^\circ, k=1+2cos⁡2θk=1+2\cos2\theta is a small positive number, and the bracket cos⁡2(Γ/2)−ksin⁡2(Γ/2)\cos^2(\Gamma/2)-k\sin^2(\Gamma/2) vanishes where cot⁡2(Γ/2)=k\cot^2(\Gamma/2)=k. This means that on each side of the design wavelength there is another wavelength at which the equivalent retardation is exactly π\pi, at the cost of a very small ripple between these points. The idea is the same as accepting an equiripple response in exchange for a wider passband in filter design.

Example. Ignoring dispersion and taking λ0=550 nm\lambda_0=550\ \mathrm{nm}, for θ=58∘\theta=58^\circ, k=0.123k=0.123, and the other two exact half-wave points are at Γ=0.785π\Gamma=0.785\pi and 1.215π1.215\pi, i.e. 700.6 nm and 452.7 nm; the maximum leakage between the two points is about 2.5×10−42.5\times10^{-4}. Taking η≥0.99\eta\ge0.99 as the criterion, the range is 517.5–587 nm for a single plate, 421–793.5 nm for θ=60∘\theta=60^\circ, and 406.5–851 nm for θ=58∘\theta=58^\circ.

Comparing three- and five-plate achromatic half-wave plates at millimeter wavelengths, Matsumura et al. cited Title's result: the three-plate combination at (0∘,58∘,0∘)(0^\circ,58^\circ,0^\circ) gives the highest broadband modulation efficiency, and near the peak the efficiency is insensitive to the angle of the middle plate [10]. They also pointed out a trade-off: at 58∘58^\circ, the phase offset of the modulated signal (which is related to the direction of the equivalent optic axis) varies more noticeably with the detection bandwidth [10]. The three-plate combination is equivalent to a linear retarder, but its equivalent optic axis does not lie along the outer plates and drifts slowly with wavelength. When a half-wave plate is used to rotate a linear polarization, this drift shows up directly as an error in the output polarization direction; for circular polarization conversion it only adds a phase to the converted light, which, as shown later, is not a problem in geometric phase devices.

Results from real devices support this principle, and the principle is independent of the spectral band. Hanany et al. made a millimeter-wave achromatic half-wave plate from three a-cut sapphire plates, with the middle plate rotated by 50.5∘50.5^\circ relative to the outer plates, and measured a modulation efficiency of 96±1.5%96\pm1.5\% at 110 GHz, compared with only 43±4%43\pm4\% for a single sapphire plate of the same thickness; the modulation efficiency was essentially unchanged for angles of incidence within 0∘0^\circ–15∘15^\circ [11]. Adding more plates broadens the bandwidth further: a nine-plate combination designed by Title using Jones matrices keeps the retardation deviation within 1∘1^\circ over 350–1000 nm [12]. The mica three-plate quarter-wave plate design given by Pancharatnam in his original paper covers 410–680 nm [8].

The difficulty with multi-plate stacks lies in fabrication. Each plate must be made and aligned separately, and the angle and thickness errors of the plates accumulate rapidly as the number of plates increases; the interfaces between several discrete elements also introduce reflections and interference [4].

Liquid crystal polymer multi-twist retarders

Liquid crystal polymers, also called reactive mesogens, are low-molecular-weight liquid crystals when coated; they can be aligned by an alignment layer just like ordinary liquid crystals, and once aligned they are polymerized with ultraviolet light and cured into a crosslinked solid film [4]. Adding a small amount of chiral dopant makes the molecules rotate uniformly through the thickness, forming a twisted layer: from the bottom to the top of the layer, the azimuth of the director (the average direction of the long molecular axes) rotates by a definite twist angle ϕm\phi_m.

A twisted layer can be regarded as a continuous stack of infinitely many extremely thin waveplates, each with its optic axis rotated by a small angle relative to the previous one; its Jones matrix is the product of the matrices of these thin plates [9]. The Pancharatnam structure changes the optic axis direction abruptly at a few discrete interfaces, whereas a twisted layer rotates the optic axis continuously.

The multi-twist retarder (MTR) proposed by Komanduri, Lawler and Escuti in 2013 stacks several twisted layers on a single substrate using only one alignment layer [4]. The key is self-alignment: each subsequent liquid crystal layer is coated onto the already cured previous layer and is aligned directly by the molecular orientation at the surface of that layer. The starting azimuth of layer m+1m+1 therefore automatically equals the ending azimuth of layer mm; no additional alignment layer is needed between layers and no layer-by-layer alignment is required, so the whole structure is a single monolithic film with a continuously varying optic axis [4]. An MTR consisting of MM layers has 2M+12M+1 design parameters: the starting angle ϕ0\phi_0 set by the alignment layer, and the twist angle ϕm\phi_m and thickness dmd_m of each layer; these parameters are determined by numerical optimization [4].

Structure and director profile of a two-layer multi-twist retarder
Figure 4. Structure of a two-layer twisted retarder (the 2TR HW-B design [4]), schematic. Left: cross-section; blue bars show the director orientation at each depth (drawn in oblique projection). Layer 1 has its starting direction set by the alignment layer and twists by 69.7∘69.7^\circ in one direction; layer 2 is aligned automatically by the top surface of layer 1 and twists back by 69.7∘69.7^\circ; both layers are 1.56 µm thick; k\mathbf k is the direction of light propagation. Right: director azimuth ψ\psi versus depth zz, increasing linearly from −3.4∘-3.4^\circ to 66.3∘66.3^\circ and returning to −3.4∘-3.4^\circ, continuous at the interface between the layers.

The two-layer half-wave design for circular polarization conversion (labeled 2TR HW-B in the paper) is: ϕ0=−3.4∘\phi_0=-3.4^\circ, both layers 1.56 µm thick, with twist angles of +69.7∘+69.7^\circ and −69.7∘-69.7^\circ [4] (Figure 4). Two layers of equal thickness with opposite twist senses form exactly the structure used earlier by Oh and Escuti for achromatic polarization gratings [13]. The three-layer design 3TR HW-B has layer thicknesses of 1.1, 2.27 and 1.1 µm and twist angles of 76.4∘76.4^\circ, 0∘0^\circ and −76.4∘-76.4^\circ [4]. The paper also gives a rule: moving to another spectral band only requires scaling the layer thicknesses proportionally, with the twist angles unchanged [4].

Figure 5 compares the leakage of several half-wave structures. To match the conditions of the paper, all curves use the birefringence dispersion of RMS10-025 [4] and are calculated by multiplying Jones matrices layer by layer, with the twisted layers sliced into thin sublayers.

Leakage of circular polarization conversion for liquid-crystal half-wave structures
Figure 5. Fraction 1−η1-\eta of circularly polarized light left unconverted by various liquid crystal half-wave structures (logarithmic scale, example calculation). All structures use the birefringence dispersion of RMS10-025 [4]. Grey line: single-layer half-wave plate designed for 550 nm; blue line: Pancharatnam structure of three uniform layers stacked at 0∘/58∘/0∘0^\circ/58^\circ/0^\circ; orange and red lines: the two-layer and three-layer twisted designs from the literature [4]. Total thicknesses are given in parentheses, and the dashed line marks 1−η=1%1-\eta=1\%. The dips in the curves are wavelengths of complete conversion, truncated at 10−510^{-5} in the figure.

Using η≥0.99\eta\ge0.99, the single layer (1.77 µm) covers only 526–577.5 nm. The two-layer twisted structure (total thickness 3.12 µm) covers 450.5–654 nm, a relative bandwidth of about 37%; the three-layer twisted structure (total thickness 4.47 µm) covers 404.5–784 nm, a relative bandwidth of about 64%. With the same dispersion, three uniform layers stacked at 0∘/58∘/0∘0^\circ/58^\circ/0^\circ cover 445–775.5 nm, close to the three-layer twisted structure.

Using ∣S3∣≥0.99|S_3|\ge0.99 as the criterion, equivalent to a leakage of no more than 0.5%, the paper gives relative bandwidths of about 37% and 75% for the two-layer and three-layer half-wave designs [4]. Recalculating with the same criterion gives narrower ranges, about 33% and 48%. The leakage curve of the three-layer design oscillates around 0.5%, and the recalculated result is very sensitive to rounding of the parameters: changing a thickness by 0.05 µm or a twist angle by a few degrees moves the recalculated bandwidth anywhere between 30% and 55%. Figure 5 is therefore meant to show the relative trends of the different kinds of structures; the performance of the specific designs should be taken from the original paper.

This comparison shows that the main advantage of MTRs is not the theoretical bandwidth for a given number of layers. The authors of the paper also concluded that for every conventional design made of multiple uniform waveplates, there is an MTR design with the same number of layers and comparable normalized bandwidth [4]. The real difference lies in fabrication: stacking a uniform liquid crystal layer at 58∘58^\circ on the previous layer requires either making a new alignment layer or fabricating a separate film and laminating it, followed by precise alignment; a twisted layer automatically inherits its direction from the top surface of the previous layer, and the angular relations are set by the chiral dopant concentration and the thickness, with no alignment needed.

Komanduri et al. reported that the twist angle and thickness of each layer can be controlled to within 1∘1^\circ and 25 nm, that the entire fabrication takes only a few minutes, and that the films can be coated on 2–6 inch substrates [4]. The two-layer achromatic quarter-wave plate they fabricated had an average output ellipticity of 0.96 over 450–650 nm, and the three-layer design 0.95 over 400–800 nm (an ellipticity of 1 means ideal circular polarization) [4]. Preliminary simulations and experimental observations indicate that these quarter-wave and half-wave designs perform consistently for angles of incidence up to at least 30∘30^\circ [4].

One point needs attention when using MTRs: because the structure is asymmetric through the thickness, it generally has no true optic axis as a whole, and its front and back faces are not interchangeable. For example, the two-layer quarter-wave design in the paper converts linear polarization into circular polarization when light enters through layer 1, and converts circular polarization back into linear polarization when light enters through layer 2; but if circularly polarized light enters through layer 1, the output is not linearly polarized [4].

Anomalously dispersive materials: letting a single layer satisfy the condition

Return to the single-plate condition Δn∝λ\Delta n\propto\lambda. If the birefringence of a material were proportional to wavelength over the entire band, Γ=2πΔn d/λ\Gamma=2\pi\Delta n\,d/\lambda would be constant and a single layer would be achromatic. This property of birefringence increasing with wavelength is called anomalous dispersion, often referred to in the display industry as reverse dispersion.

One way to achieve it is to combine positively and negatively birefringent units in the same polymer. After stretch orientation, the total birefringence of the film can be approximated as the sum of the contributions of the two kinds of units, Δn(λ)≈f+Δn+(λ)+f−Δn−(λ)\Delta n(\lambda)\approx f_{+}\Delta n_{+}(\lambda)+f_{-}\Delta n_{-}(\lambda), where Δn−<0\Delta n_{-}<0 and ff denotes volume fraction. If the magnitude of the negative contribution grows faster than the positive contribution as the wavelength decreases, the two cancel more and more toward short wavelengths, so the total birefringence decreases as the wavelength decreases, exhibiting anomalous dispersion.

Uchiyama and Yatabe synthesized copolycarbonates from bisphenol A and fluorene-containing monomers and found that stretched films exhibit anomalous dispersion for fluorene-unit volume fractions in the range 0.65–0.80; the shape of the dispersion is set mainly by the copolymer ratio and is insensitive to the stretching conditions [14]. Their later review pointed out that broadband behavior appears only within a narrow composition range near the zero point of the birefringence; broadband retardation films of copolycarbonate based on this principle have been industrialized for polarization conversion in flat-panel displays, replacing designs that previously required a combination of two retardation films with a single film [15].

The limitations of this route also come from the principle itself. The broadband behavior is obtained by near-cancellation of two contributions, so the composition window is narrow and the net birefringence is small; moreover, Δn∝λ\Delta n\propto\lambda can hold only approximately over a limited band. Komanduri et al. mentioned that a single layer of an anomalously dispersive liquid crystal mixture has a normalized bandwidth of about 15%, roughly half that of a two-layer MTR; they also pointed out that the two approaches can be combined by using anomalously dispersive liquid crystals in an MTR [4].

Specifications: retardation error, bandwidth, viewing angle and temperature

When comparing or selecting achromatic waveplates (for example a broadband achromatic waveplate), the first step is to be clear about how each specification is defined, since different publications often use different criteria.

Retardation error. The most direct specification is how far the equivalent retardation deviates from the target value. For circular polarization conversion, it is related to the leakage by 1−η=sin⁡2(ε/2)1-\eta=\sin^2(\varepsilon/2): a leakage of 1%1\% corresponds to a retardation error of about 11.5∘11.5^\circ, 0.5%0.5\% to about 8.1∘8.1^\circ, and an error of 1∘1^\circ causes a leakage of only about 7.6×10−57.6\times10^{-5}. For quarter-wave plates, the ellipticity of the output light or the Stokes parameter S3S_3 is commonly used; when a half-wave plate is used to rotate linear polarization, the drift of the equivalent optic axis with wavelength also matters [10].

Bandwidth. This is usually written as the ratio of the wavelength range Δλ\Delta\lambda satisfying a given criterion to the center wavelength λ0\lambda_0. Different criteria can give very different numbers: Komanduri et al. used ∣S3∣≥0.99|S_3|\ge0.99 for half-wave designs, equivalent to a leakage of no more than 0.5% [4], whereas Figure 5 in this article uses 1%. When comparing bandwidth data from different sources, first convert them to the same criterion.

Viewing angle. Oblique incidence changes the optical path and effective birefringence in each layer, by an amount that depends on the thickness and total retardation of the layer. Compound zero-order waveplates and two-material combinations made of thick crystal plates are about as sensitive to the angle of incidence as multi-order waveplates of the same thickness [6]; combining positive and negative uniaxial crystals reduces this sensitivity [6]. Liquid crystal polymer films are only a few micrometers thick, and the result that MTRs perform consistently for angles of incidence up to at least 30∘30^\circ is still preliminary [4].

Temperature. Birefringence varies with temperature. The net retardation of a compound zero-order waveplate is set by the thickness difference of the two plates, so its temperature response is the same as that of a true zero-order waveplate [6]; in a two-material combination, the two materials have different temperature coefficients, and the temperature-induced changes in the roughly 10-wave retardations of the two plates generally do not cancel, so such combinations are temperature-sensitive [4]. The temperature behavior of liquid crystal polymer devices depends on the specific material and must be evaluated separately from material data.

Alignment and interfaces. The performance of discrete multi-plate structures is limited by the angle and thickness tolerances of the plates, which become harder to guarantee as the number of plates grows; multiple interfaces also introduce reflections and interference [4]. In an MTR, the directions between layers are guaranteed by self-alignment, and the tolerances come mainly from control of the twist angles and thicknesses [4].

The table below summarizes the characteristics of the four approaches; the structures listed are examples from this article or designs from the literature.

Approach Basis of compensation Example structure Main limitations
Two-material combination Two materials with different dispersions, zero net group delay difference Quartz 578 µm and MgF₂ 470 µm, optic axes orthogonal Thick; sensitive to viewing angle and temperature; residual second-order error
Pancharatnam multi-plate Same material, arranged at angles so the error rotation axes close Three identical half-wave plates, 0∘/58∘/0∘0^\circ/58^\circ/0^\circ Plate-by-plate fabrication and alignment, error accumulation, interface reflections
Multi-twist (MTR) Twisted layers rotate the optic axis continuously; parameters optimized numerically Two layers of 1.56 µm each, twists of ±69.7∘\pm69.7^\circ Front and back not interchangeable; performance depends on material dispersion
Anomalously dispersive material Single-layer birefringence approximately proportional to wavelength Copolycarbonate film with positively and negatively birefringent units Narrow composition window, limited bandwidth

Relation to broadening the bandwidth of geometric phase devices

Geometric Phase (PB Phase): How Liquid Crystals Shape Phase in a Flat Layer explains that a liquid crystal half-wave layer with optic axis azimuth α(x,y)\alpha(x,y) converts left-handed input into right-handed light and adds a geometric phase of +2α+2\alpha, or −2α-2\alpha for right-handed input; the conversion efficiency is η=sin⁡2(Γ/2)\eta=\sin^2(\Gamma/2), and the unconverted part becomes the zero order in a polarization grating and unfocused background light in a PB lens. The geometric phase itself is independent of wavelength; wavelength affects only the efficiency, through Γ\Gamma. Broadening the bandwidth of geometric phase devices therefore comes down, first of all, to making the local half-wave plate at every point an achromatic half-wave plate.

When the single layer is replaced by a compound structure, one thing must be confirmed: whether the geometric phase is still ±2α\pm2\alpha. The answer is yes, as long as the entire stack at each point rotates together by α\alpha. Let the Jones matrix of a stack be JJ; after the whole stack rotates by α\alpha, it becomes R(−α) J R(α)R(-\alpha)\,J\,R(\alpha), where R(α)R(\alpha) is the coordinate rotation matrix. In the circular polarization basis, R(α)R(\alpha) is diagonal, with two diagonal elements that are phase factors of the form e±iαe^{\pm i\alpha}. After multiplying once on each side, the off-diagonal elements connecting the two handednesses (the conversion terms) acquire e±2iαe^{\pm2i\alpha}, while the diagonal elements (the leakage terms) are unchanged. This conclusion does not depend on how many layers the stack contains or whether they are twisted.

The stack itself also adds an intrinsic phase to the converted light. This phase varies with wavelength, but it is the same at every position on the device, so it is only an overall constant phase and does not change the shape of the wavefront.

Example. For the 2TR HW-B structure, Jones-matrix calculation in this article shows that for left-handed input, the intrinsic phase of the converted light is 78.1∘78.1^\circ at 450 nm and −4.6∘-4.6^\circ at 550 nm; after the whole stack is rotated by 20∘20^\circ, the phase at both wavelengths increases by exactly 40∘40^\circ, i.e. 2α2\alpha.

Self-alignment satisfies exactly the requirement that "the entire stack rotates together". When an MTR is coated on a patterned alignment layer, the alignment layer sets the starting angle ϕ0+α(x,y)\phi_0+\alpha(x,y) at every point and the subsequent layers inherit it automatically, so the entire local stack at every point is rotated by α(x,y)\alpha(x,y) [4]. Realizing a Pancharatnam structure with discrete uniform layers would require a separate patterned alignment layer for each layer, with the patterns of the layers offset from each other by exactly a fixed angle, which is very difficult to fabricate. The achromatic polarization grating of Oh and Escuti, made by stacking two chiral polarization grating layers with opposite twist senses, achieved a diffraction efficiency of about 100% in both theory and experiment, with an operating bandwidth Δλ/λ0\Delta\lambda/\lambda_0 of about 56% [13]. The structure and steering behavior of polarization gratings are covered in Liquid Crystal Polarization Gratings (LCPG): How Electrical Beam Steering Works.

The local-waveplate approximation used here requires the spatial period of the alignment pattern to be much larger than the film thickness; otherwise the molecular orientations of neighboring regions influence each other and the actual structure departs from the design.

It is also important to distinguish what an achromatic waveplate does and does not solve. It brings the conversion efficiency close to 1 over a broad band, reducing zero-order leakage or background light accordingly; but the deflection angle of a polarization grating still obeys sin⁡θ=λ/Λ\sin\theta=\lambda/\Lambda, and the focal length of a PB lens is still inversely proportional to wavelength. This diffractive dispersion comes from the phase gradient itself, not from the retardation, and must be compensated separately; see Achromatic Liquid Crystal Lenses: How Chromatic Aberration in Diffractive Lenses Is Corrected. How achromatic waveplates and achromatic liquid crystal devices are used in imaging and polarization control systems is covered in Applications of Achromatic Liquid Crystal Devices: Full-Color Displays and Broadband Polarization Control.

References

[1] E. Hecht. Optics, 5th ed. Pearson, 2017. ISBN 978-0-13-397722-6

[2] G. Ghosh. Dispersion-equation coefficients for the refractive index and birefringence of calcite and quartz crystals. Optics Communications, 163(1-3): 95–102, 1999. DOI: 10.1016/S0030-4018(99)00091-7

[3] M. J. Dodge. Refractive properties of magnesium fluoride. Applied Optics, 23(12): 1980, 1984. DOI: 10.1364/AO.23.001980

[4] R. K. Komanduri, K. F. Lawler, M. J. Escuti. Multi-twist retarders: broadband retardation control using self-aligning reactive liquid crystal layers. Optics Express, 21(1): 404–420, 2013. DOI: 10.1364/OE.21.000404

[5] P. Hariharan. Achromatic and apochromatic halfwave and quarterwave retarders. Optical Engineering, 35(11): 3335–3337, 1996. DOI: 10.1117/1.601074

[6] P. D. Hale, G. W. Day. Stability of birefringent linear retarders (waveplates). Applied Optics, 27(24): 5146–5153, 1988. DOI: 10.1364/AO.27.005146

[7] S. Pancharatnam. Achromatic combinations of birefringent plates. Part I: An achromatic circular polarizer. Proceedings of the Indian Academy of Sciences - Section A, 41(4): 130–136, 1955. DOI: 10.1007/BF03047097

[8] S. Pancharatnam. Achromatic combinations of birefringent plates. Part II: An achromatic quarter-wave plate. Proceedings of the Indian Academy of Sciences - Section A, 41(4): 137–144, 1955. DOI: 10.1007/BF03047098

[9] A. Yariv, P. Yeh. Optical Waves in Crystals: Propagation and Control of Laser Radiation. Wiley, 2002 (Wiley Classics Library reprint; first published 1984). ISBN 978-0-471-43081-0

[10] T. Matsumura, S. Hanany, P. Ade, B. R. Johnson, T. J. Jones, P. Jonnalagadda, G. Savini. Performance of three- and five-stack achromatic half-wave plates at millimeter wavelengths. Applied Optics, 48(19): 3614, 2009. DOI: 10.1364/AO.48.003614

[11] S. Hanany, J. Hubmayr, B. R. Johnson, T. Matsumura, P. Oxley, M. Thibodeau. Millimeter-wave achromatic half-wave plate. Applied Optics, 44(22): 4666, 2005. DOI: 10.1364/AO.44.004666

[12] A. M. Title. Improvement of birefringent filters. 2: Achromatic waveplates. Applied Optics, 14(1): 229, 1975. DOI: 10.1364/AO.14.000229

[13] C. Oh, M. J. Escuti. Achromatic diffraction from polarization gratings with high efficiency. Optics Letters, 33(20): 2287, 2008. DOI: 10.1364/OL.33.002287

[14] A. Uchiyama, T. Yatabe. Control of wavelength dispersion of birefringence for oriented copolycarbonate films containing positive and negative birefringent units. Japanese Journal of Applied Physics, 42(11): 6941–6945, 2003. DOI: 10.1143/JJAP.42.6941

[15] A. Uchiyama, Y. Ono, Y. Ikeda, H. Shuto, K. Yahata. Copolycarbonate optical films developed using birefringence dispersion control. Polymer Journal, 44(10): 995–1008, 2012. DOI: 10.1038/pj.2012.52